Causes and solutions of top whiteness in injection molding products

Release time:2021-08-16

When the plastic parts of injection products are ejected from the mold, if the ejector pin is used, the ejector rod will often leave deep or shallow marks on the plastic parts. If these traces are too deep, the so-called top white phenomenon will appear. In serious cases, the so-called top explosion will occur when the plastic parts are pushed through.


The main reason for the whiteness of plastic parts is that the product has a large mold adhesion force, and the ejection part on the plastic parts causes white marks at the ejection part of the ejector rod. The specific reasons and improvement methods are as follows:


1. Back mold temperature is too low or too high: adjust the appropriate mold temperature.


2. Too fast ejection speed: slow down the ejection speed.


3. With demoulding chamfer: overhaul the mold (polishing).


4. The ejection of finished products is unbalanced (the ejection leaf spring is broken): repair the mold (make the ejection balanced).


5. Insufficient number of thimbles or improper position: increase the number of thimbles or change the position of thimbles.


6. Vacuum occurs in the mold during demoulding: clean the dirt in the ejector pin hole to improve the air inlet effect.


7. The finished bone and column positions are rough (inverted): polish each bone and column position.


8. High injection pressure or holding pressure: reduce the pressure appropriately.


9. The demoulding angle of the finished mold is too small: increase the demoulding angle of the rear mold.


10. Improper action time or position of side slider: repair the mold (make the core pulling action normal).


11. Ejection area is too small or ejection speed is too fast: increase the ejection area or slow down the ejection speed.


12. The injection speed of the last section is too fast (Burr): slow down the injection speed of the next section.


These are the reasons and solutions for the whitening of injection molded products.

Copyright: Shenzhen Zhongyuan Plastic Co., Ltd. | mold processing customized manufacturer. If you want to know the processing price of the factory, how much is it, and which is good, please contact us Yue ICP Bei No. 17060480
精品国品一二三产品区别在线观看 | 日本不卡一区二区三区| 一级午夜福利视频免费区| 国产精品啪啪啪免费观看 | 中文成人无字幕乱码精品区| 一个人深夜激情在线观看| 高清黑人中出在线小视频| 亚洲阿v天堂网2021| 午夜久久久久久久电影网| 国产日产久久高清欧美一区ww| 99在线儿免费观看视频| 18禁精品一区二区三区| 绝色爆乳女教师在线观看| 午夜爱爱免费视频无遮挡| 久久精品女?的天堂AV| 日韩性无码国产精品专区| 久久99精品国产综合毛片| 在线日本欧美一区二区三区 | 国产精品久久久久一区二区三区共| xxxxx在线免费观看| 国产精品无码无卡免费观| 久久久无码国产| 无码八a片人妻少妇久久| 欧美大几吧网站在线观看| 色婷婷在线视频免费播放| 国产99视频精品免费视频76| 亚洲欧美日韩中文加勒比| 精品国产高清一区二区三区| 免费在线观看欧美小黄片| 亚洲4438丁香五月天| 男插女激烈视频在线观看| 亚洲一区二区中文字幕av| 成人在线午夜你懂的视频| 18禁动画在线免费观看| 亚洲性AV综合在线观看| 久久中文字幕第一页在线| 欧美亚洲三级片| 操爽了手机在线免费观看| 啊啊啊不要好棒视频在线| 老女人在线精品视频免费| 亚洲一区无码精品色变态|